Defects and preventive measures of stamping and stretching parts
Time : 2023-08-30 Click count : 2648

1. Reasons for waste generation:

A. Poor quality of raw materials;

B. Improper installation, adjustment, and use of molds;

C. The worker did not feed the strip correctly along the positioning or did not ensure that the strip was fed with a certain gap;

D. Due to long-term use of the mold, there may be changes in gaps or wear on the working and guiding components of the mold;

E. Due to prolonged impact and vibration, the fastening parts of the mold become loose, causing a relative change in the installation position of the mold;

F. The operator's negligence did not follow the operating procedures.


2. The main measures to prevent waste are:

A. Raw materials must meet the specified technical conditions (strictly inspect the specifications and brands of raw materials, and conduct laboratory tests on workpieces with high requirements for dimensional accuracy and surface quality when conditions permit)

B. All aspects specified in the process specifications should be strictly followed comprehensively;

C. The tools and equipment used, such as presses and molds, should ensure that they work under normal working conditions;

D. Establish a strict inspection system during the production process, which requires a thorough inspection of the first stamped part. Only after passing the inspection can they be put into production. At the same time, inspection should be strengthened, and accidents should be dealt with in a timely manner;

E. Adhere to the civilized production system, for example, workpieces and blanks must be transported using appropriate workstation equipment, otherwise the surface of the workpiece will be crushed and scratched, affecting the surface quality of the workpiece;

F. During the stamping process, the cleanliness of the mold cavity should be ensured, and the orderly arrangement of workpieces after processing in the workplace should be neat.


3. Causes of burrs on punched parts

A. The punching gap is too large, too small, or uneven;

B. The cutting edge of the working part of the mold becomes dull;

C. Due to long-term vibration impact, the centerlines of the convex and concave molds change, and the axes do not coincide, resulting in one-sided burrs.

measures:

1) Ensure the machining accuracy and assembly quality of convex and concave molds, ensure the verticality of convex molds, withstand lateral pressure, and ensure the rigidity of the entire mold;

2) When installing the convex mold, ensure that the gap between the convex mold and the concave mold is correct, and firmly install the convex mold and the concave mold on the mold fixing plate. The end faces of the upper and lower molds should be parallel to the worktable of the press.

3) The requirements for the press include good rigidity, minimal elastic deformation, high track accuracy, and high parallelism between the pad and slider;

4) Require the pressure machine to have sufficient punching force.

The allowable height of burrs on the cut surface of punched parts

Punched sheet thickness>0.3>0.3-0.5>0.5-1.0>1.0-1.5>1.5-2.0

New trial mold burr height ≤ 0.015 ≤ 0.02 ≤ 0.03 ≤ 0.04 ≤ 0.05

The allowable burr height in production is ≤ 0.05 ≤ 0.08 ≤ 0.10 ≤ 0.13 ≤ 0.15


4. Reasons for warping and deformation of punched parts:

There are clearance forces and reaction forces on a straight line that do not generate torque. When the gap between the punch and the die is too large, the edge of the die has a conical shape, or when the contact area between the ejector and the workpiece is too small, warping deformation will occur

measures:

A. Reasonably choose the punching gap;

B. In the mold structure, a certain amount of pressure is required to increase the plane contact between the pressing plate (or support plate) and the pressing plate;

C. Check the concave die blade. If a reverse taper is found, the cutting edge of the die must be trimmed correctly.

D. When the shape of the punched part is complex and there are many inner holes, if the cutting force is uneven, the pressing force will increase. Before punching, press the strip tightly or use a high-precision press to punch it.

E. Before punching the sheet metal, it should be leveled. If the warping cannot be removed, the punched workpiece can be re leveled using a leveling mold.

F. Regularly clean the dirt inside the mold cavity, lubricate the surface of the thin sheet material, and install oil vent holes on the mold structure.


5. During punching, the accuracy of the outer edge and inner hole of the punched part decreases, and the size changes.

reason:

The position of positioning pins, blocking pins, etc. has changed or worn out excessively;

The operator's carelessness caused the material to move back and forth during feeding;

The dimensional accuracy of the strip material is low, too narrow and too wide, making it difficult to deliver to the designated location. If the strip material moves back and forth in the guide plate, the punching hole of the workpiece will have a significant deviation from the front and rear positions of the outer shape.


6. Reasons for non-conforming bending dimensions and shapes of parts

A. The rebound of the material causes the product to be unqualified

Measures to reduce rebound:

Choose stamping materials with stable mechanical properties, high elastic modulus, and low yield point;

Add calibration program and use calibration bending instead of free bending;

Before bending, the material should be annealed to soften the cold work hardened material before bending into shape;

If there is shape deformation during stamping, it is difficult to remove; Then change or adjust the slope of the convex and concave molds, and the gap between the convex and concave molds should be equal to the minimum material thickness.

Increase the contact area between the concave mold and the workpiece, and reduce the contact area between the convex mold and the workpiece.

Reduce the impact of rebound by overcorrecting.

B. If the locator is worn and deformed, causing inaccurate positioning of the strip, a new locator must be replaced.

C. In non guided bending molds, improper adjustment of the bottom dead center position of the press slide during adjustment on the press can also result in the shape and size of the bent part being non-conforming.

D. If the pressing device of the mold malfunctions or does not work at all, it is necessary to readjust the pressing force or replace the pressure spring to make it work normally.


7. Cracks appear at the bending part of the bent part (the internal stress in the bending deformation zone exceeds the material strength limit)

A. Removing burrs outside the curved area can lead to stress concentration in that area,

1) Reduce bending deformation

2) Remove burrs from the area

3) Place the side with burrs inside the curved area

B. When bending workpieces, it is best to make the bending direction perpendicular to the fiber direction (rolling direction) of the material.

C. The bending radius should not be too small, and if the quality allows, the fillet radius should be increased as much as possible.

D. The surface of the bent blank should be smooth, without obvious protrusions or scars.

E. Intermediate annealing process is used to remove internal stress during bending, and softening bending rarely produces cracks.

F. When bending, larger bending parts must be coated with lubricant to reduce friction during bending.


8. Deviation of bent parts during bending process

During the bending process, when the blank slides along the surface of the concave mold, it will experience frictional resistance. If the frictional resistance on both sides of the blank is significantly different, the blank will move towards the side with greater frictional resistance.

measures:

1) Asymmetric bending parts are formed by symmetrical bending (single-sided bending parts are cut after two symmetrical bends)

2) Add an elastic compression device on the bending mold to compress the billet and prevent it from moving during bending.

3) Utilize internal holes and external positioning forms to ensure accurate positioning.


9. Reasons and solutions for surface scratches on curved parts.

A. When continuously bending soft materials such as copper and aluminum alloys, metal particles or slag are prone to adhere to the surface of the working area, causing significant scratches on the parts. At this time, it is necessary to carefully analyze and study the shape and lubricating oil of the working parts, and it is best to avoid particles and slag on the blank, which can cause scratches.

B. When the bending direction is parallel to the rolling direction of the material, cracks will appear on the surface of the workpiece, reducing the surface quality of the workpiece. When two or more parts are bent, ensure that the bending direction is as close as possible to the rolling direction.

C. When the burr surface is bent as the outer surface, the parts are prone to cracking and scratching; Therefore, the burr surface should be considered as a curved inner surface.

D. The fillet radius of the concave mold is too small, and there are impact marks on the curved part. Polishing the concave mold and increasing the fillet radius of the concave mold can avoid wear on bent parts.

E. The gap between the convex and concave molds should not be too small, otherwise it will cause thinning and wear. Regularly check the changes in mold clearance during stamping.

F. If the depth of the convex mold entering the concave mold is too large, there may be scratches on the surface of the part. Therefore, while ensuring that it is not affected by rebound, the depth of the convex mold entering the concave mold should be appropriately reduced.

G. In order to meet the precision requirements of the parts, bottom pressing bending molds are often used. When bending, the springs, locating pin holes, support plates, and return holes on the pressing plate will be pressed into indentations and should be adjusted.


10. What is the reason for the change in the position of the blank hole during bending? How to exclude

A. The position and size of the hole are incorrect, resulting in thinning due to bending and stretching

Measures: Strictly control the bending radius, bending angle, and material thickness; Trim the neutral layer of the material so that the depth of the convex mold entering the concave mold and the depth of the convex and concave molds are appropriately consistent.

B. Reasons for non concentric holes

1) Insufficient bending height. 2) The blank slides. 3) Rebound. 4) The curved plane exhibits undulations.

measures:

1) Ensure the correct left and right bending height.

2) Correct the worn positioning pins and plates.

3) Reduce rebound and ensure the parallelism and flatness of the two curved surfaces.

4) Change the process route, first bend and correct before punching.

C. The bending curve is not parallel to the centerline of the two holes, and the part with a bending height less than the minimum bending height shows an outward opening shape after bending.

measures:

1) When bending, the minimum bending height H (H ≥ R 2t t material thickness R bending radius) should be ensured.

2) Change the shape of the processed parts and remove parts with a bending height less than the minimum without affecting their use.

D. Holes near curved lines are prone to deformation.

measures:

1) When designing bent parts, ensure that the edge distance X from the bent part to the hole is greater than a certain value X ≥ (1.5-2.0) t t t of the bent sheet thickness.

2) Designing auxiliary holes in the bending area to absorb bending deformation stress can prevent hole deformation near the bending curve. Generally, the scheme of bending first and punching later is adopted.


11. After bending, the bent parts show significant thinning

A. The bending radius is too small relative to the plate thickness value (r/t>3 right angle bending). Generally, increasing the bending radius is used.

B. Multi angle bending makes the bent part thinner and larger. In order to reduce thinning, the single angle multi process bending method should be used as much as possible.

C. When using a pointed convex mold, the convex mold enters the concave mold too deeply, significantly reducing the thickness of the bent part.


12. Reasons and prevention of flange wrinkling during deep drawing process of deep drawn parts

reason:The edge pressure on the flange is too small to resist excessive tangential compressive stress; And it causes tangential deformation, resulting in the formation of folds after losing stability. Thinner materials are also prone to wrinkle formation.

measures:Increase the edge pressure of the edging ring and appropriately increase the thickness of the material.


13. Reasons and prevention of wall cracking in deep drawn parts

reason:

A. Excessive radial tensile stress of the material during stretching;

B. The radius of the concave mold fillet is too small,

C. Poor lubrication during deep drawing;

D. The plasticity of raw materials is poor.

measures:

1) Reduce the edge pressure.

2) Increase the fillet radius of the concave mold.

3) Proper use of lubricants.

4) Choose materials with better performance or add annealing processes in the workshop.


14. The bottom of the deep drawn part is cracked by pulling

The reason is that the fillet radius of the concave mold is too small, which causes the material to be cut. (Usually occurring in the early stage of deep drawing) Increasing the fillet radius of the concave die reduces the surface roughness of its smooth transition, usually Ra<0.2 μ m.


15. The edges of the deep drawn parts are uneven and wrinkled.

reason:The blank and the center of the convex concave die are not in a straight line or the material thickness is uneven. The radius of the concave die corner is uneven with the gap between the convex concave die (if the radius of the concave die corner is too large, the edge pressing ring and the edge pressing ring will separate in the final stage of deep drawing, and the material that does not cross the corner cannot be pressed into the edge pressing ring and wrinkled before being pulled into the concave die to form mouth edge wrinkles).

measures:Repositioning the die, before putting it into production, adjust the fillet radius of the concave die and the clearance between the convex and concave dies to make them uniform in size (reducing the fillet radius of the concave die or using an arc-shaped edge pressing ring device can remove wrinkles)


16. Reasons and preventive measures for wrinkling at the waist during deep drawing of conical or hemispherical parts:

reason:At the beginning of deep drawing, most of the material is in a suspended state, with too little edge pressure, too large fillet radius of the die, or excessive use of lubricant. The radial tensile stress decreases, and the material loses stability under tangential compressive stress, resulting in wrinkles.

measures:Increase the edge pressure or adopt a rolled rib structure, reduce the fillet radius of the concave die or slightly increase the material thickness.


17. Reasons and preventive measures for drawing marks on the surface of deep drawn parts

reason:

A. If there are sharp scratches on the surface of the convex or concave mold, resulting in corresponding tensile marks on the surface of the workpiece, the surface should be polished or buffed.

B. The gap between the convex and concave molds is too small or uneven, causing scratches on the surface of the workpiece during deep drawing. At this time, the gap between the convex and concave molds should be adjusted until it is suitable.

C. The concave die has a rough rounded surface, and the workpiece surface is scratched during stretching. At this point, the radius of the rounded corners of the concave mold should be polished and smoothed.

D. During stamping, impurities are mixed into the working surface or material surface of the die due to uncleanliness, which damages the surface of the workpiece. Therefore, the surface of the convex and concave molds must always be kept clean during material pulling, and the blank must be wiped before pulling;

E. When the hardness of the convex and concave molds is low, metal shavings will adhere to their surfaces, and there will also be stretch marks on the surface of the deep drawn workpiece. Therefore, in addition to increasing the hardness of the convex concave die surface, even if the remaining metal waste is removed, the surface of the convex concave die should always be inspected.

F. Poor quality lubricants can also increase the surface roughness of deep drawn workpieces. In this case, lubricants suitable for deep drawing processes should be used, and if necessary, the lubricant should be filtered before use. Thus preventing impurities from entering and damaging the surface of the workpiece.


18. What is the reason for the unevenness of the straight wall of the deep drawn part?

reason:

A. There are no ventilation holes designed and manufactured on the convex mold, so the surface of the convex mold will deform due to compressed air, resulting in unevenness. In this case, ventilation holes must be added.

B. The rebound of the material can also cause unevenness on the surface of the deep drawn workpiece, and finally, a shaping process needs to be added.

C. The gap between the convex and concave molds is too large, making it difficult to flatten during deep drawing. At this time, the gap must be uniformly adjusted.

News Related news
国产一线二线在线观看 | 在线国产福利 | 99人妻少妇精品视频一区 | 国产女主播喷水高潮网红在线 | 欧美日韩在线精品 | 日韩成人av免费在线观看 | 国产精品人人妻人人爽 | 青在线视频 | 精品欧美一区二区三区久久久 | 国产日韩精品中文字无码 | 日本大尺度床戏揉捏胸 | 色婷婷婷| 亚洲综合成人在线 | 国产亚洲高清视频 | kk视频在线观看 | 免费黄色入口 | 成人精品视频一区 | 国产精品久久AV无码 | 日本免费无人高清 | 妖精视频一区二区三区 | 国产精品人人妻人人爽人人牛 | 人人射人人爽 | 日韩在线视频免费 | 欧洲成人在线视频 | 日韩在线视频播放 | 99久久99| 午夜剧场免费看 | 亚洲天堂美女 | 色妞视频| 韩国一区二区三区视频 | 日韩av在线中文字幕 | 男男play呻吟动漫网站 | www.九九九 | 巨茎人妖videos另类 | 91精品欧美| 成人免费观看网址 | 日产电影一区二区三区 | 国产女女调教女同 | 女人张开双腿让男人捅 | 激情午夜视频 | 蜜臀在线播放 | 欧美性插动态图 | av毛片在线看 | 老太婆av| 国产激情一区二区三区 | 亚洲激情另类 | 在线亚洲区 | 一起操17c| 成人免费网站www网站高清 | 美女aaa| 亚洲人一区二区三区 | 丰满大乳国产精品 | 91色爱| 亚洲成人av片 | 久久99精品国产91久久来源 | 中文字幕乱码亚洲精品一区 | 国产盗摄视频在线观看 | 天天爽夜夜爽夜夜爽 | 日本特黄一级 | 影音先锋蜜桃 | 国产波霸爆乳一区二区 | 日本特黄色片 | 豆花视频在线 | 日韩a在线播放 | 精品人妻无码一区二区三区蜜桃一 | 香蕉网站在线 | 成年网站 | 中文字幕 成人 | 永久免费在线 | 女同另类之国产女同 | 激情婷婷六月天 | 国产第一页在线观看 | 日韩一区二区免费视频 | 日日好av | 青青青久久久 | 无人在线观看高清视频 | 亚洲区小说区图片区 | 色欲无码人妻久久精品 | 一区精品视频 | 免费a级黄色片 | 韩国中文字幕hd久久精品 | 国内三级在线 | www.爱色av.com| 91高清视频在线观看 | 色婷婷综合久久久久中文 | 91成年版 | 黄色三级片毛片 | 五月天婷婷爱 | 久久中文免费视频 | 91在线国产观看 | 超碰人人91| 美女张开腿让人桶 | 玖玖精品国产 | 瑟瑟视频在线观看 | 天天干干干干干 | 国产一级片麻豆 | 色婷久久 | 二级毛片视频 | 国产精品视频一二三区 | 手机av免费 | 成a人片亚洲日本久久 | 欧美第一精品 | 国产精品自拍在线观看 | 国产福利在线观看视频 | 网站免费视频www | 欧洲在线视频 | 成人毛片一区二区三区 | 国产精品卡一卡二 | 日日cao | 91蝌蚪91九色白浆 | 51成人精品网站 | 嫩草精品| 色呦呦网站在线观看 | 男女激情网 | 四虎黄色影视 | 亚洲精品在线免费播放 | 波多野结衣高清在线 | 欧美乱插 | 熟女俱乐部五十路六十路av | 黄网站免费看 | 中日韩中文字幕一区二区 | 黑人操亚洲女 | 日韩精品一二区 | 久久人妻无码aⅴ毛片a片app | av动漫天堂 | 精品免费视频一区二区 | 久久精品99国产精品日本 | 久久高清毛片 | 中文字幕avav| 亚洲香蕉网站 | 淫欲少妇 | 99久久综合网 | 免费av视屏| 黄色av免费在线看 | 国内精品视频一区 | 国产超碰人人 | 姑娘第5集高清在线观看 | 国产青草视频 | 欧美成人黄色网 | 日日精品| 日本肉体xxxx裸体137大胆图 | 精品视频一区二区三区 | exo妈妈mv在线播放高清免费 | 日韩一区二区在线看 | 欧美性啪啪 | 邻居校草天天肉我h1v1 | 青青久在线| 日本护士做爰视频 | 日韩欧美中文字幕一区二区 | 男人的天堂a在线 | 美女赤身免费网站 | www.天天操.com | 欧美 日韩 国产 在线观看 | 免费黄色片视频 | 波多野在线播放 | 精品国产乱码久久久久久婷婷 | 天天摸天天干天天操 | 国产精品伦一区二区三级视频 | 色哟哟在线观看视频 | 欧美aa| 久久精品福利 | 欧美一级片免费观看 | 中文字幕第80页 | 梦梦电影免费高清在线观看 | 打开免费观看视频在线 | 欧美1页 | 国产在线精品视频 | 黄色va| 在线黄色网 | 无码人妻精品一区二区三区蜜桃91 | 特级淫片裸体免费看冫 | 依依成人在线 | 亚洲乱亚洲 | 欧美群妇大交群 | 亚洲自拍色 | 青草视频在线看 | 日韩在线精品视频一区二区涩爱 | 欧美午夜性生活 | 国产乱码精品一区二区三区亚洲人 | 97网站| 欧美精品一级二级 | 男人午夜视频 | 777久久| 天天躁狠狠躁狠狠躁夜夜躁68 | 夜夜草av| 懂色aⅴ一区二区三区免费 国产精品无码久久av | 天天插伊人 | 亚洲热av| 天天cao在线| 国产一级片在线 | aaa级片| 欧美亚洲另类小说 | 亚洲第一网址 | 天天躁夜夜操 | 18成人免费观看视频 | 成人午夜视频一区二区播放 | 欧美精品手机在线 | 亚洲国产成人va在线观看天堂 | 成人做爰免费视频免费看 | 91九色porny视频 | 欧美激情精品久久 | 人妻少妇精品无码专区 | 少妇太紧太爽又黄又硬又爽 | 国产成人精 | 国产美女视频91 | 小明看国产 | 国产一区91| 欧美精品videos | 精品少妇一区二区三区密爱 | 午夜在线影院 | 无码精品国产一区二区三区 | 强伦人妻一区二区三区视频18 | 日本一区二区在线不卡 | 日韩福利一区二区 | 成人激情片 | 精品久操| 韩国中文字幕hd久久精品 | 丰满人妻中伦妇伦精品app | 欧美激情啪啪 | 夜夜狠 | 综合色区 | 伊人资源 | 日韩在线视频免费 | 国产成人免费在线视频 | 怡红院精品视频 | www.777奇米影视 | 91av片| jizz一区 | 91在线网站 | 一级中国毛片 | 黄色国产免费 | 久草免费在线视频 | 美女黄色在线观看 | 噼里啪啦动漫 | 亚洲成人系列 | 欧美天堂网站 | 日本中文字幕观看 | 91精品国产91久久久久久 | 国产福利一区二区视频 | 武林美妇肉伦娇喘呻吟 | xxxxx在线视频 | 亚洲男女视频 | 国产女人与zoxxxx另类 | 五月激情视频 | 强开小嫩苞一区二区三区网站 | 激情六月色 | 永久精品网站 | 亚洲欧美日韩久久 | 在线观看国产亚洲 | 天天插天天干 | 久久久久在线 | 在线看成人片 | 亚洲成人精品在线 | 亚洲大片免费 | 九月婷婷丁香 | 色呦呦网| 欧美怡红院视频 | 亚洲人 女学生 打屁股 得到 | 男女午夜激情视频 | 国产香蕉97碰碰碰视频在线观看 | 99re在线视频 | 美女三级视频 | 日本五十肥熟交尾 | 羞羞色院91蜜桃 | 欧美一级免费在线观看 | 欧美人体视频一区二区三区 | 精品在线你懂的 | 成人性做爰aaa片免费看不忠 | 黄色录像a级片 | 亚洲av无码专区国产乱码不卡 | 50部乳奶水在线播放 | 亚洲逼| 动漫女生光屁股 | 日韩成人动漫在线观看 | 26uuu成人网 五月天精品在线 | 香蕉视频官网在线观看 | 精品国产无码在线观看 | 一级国产精品 | 成人三级电影网站 | 丝袜+亚洲+另类+欧美+变态 | 亚洲无码国产精品 | 人乳喂奶hd无中字 | 国产欧美日韩久久 | 香蕉传媒 | 性人久久久久 | 免费在线观看网址入口 | 中文字幕一区二区三区免费 | 婷婷激情综合网 | 成人在线观看www | 国产精品毛片一区二区三区 | 97香蕉碰碰人妻国产欧美 | 国产噜噜噜噜噜久久久久久久久 | 91好色先生 | 国产专区一区二区三区 | 国产任你操 | 精品国产欧美一区二区三区成人 | 精品久久人人 | 黄瓜视频色 | 伊人色播 | 久久理论 | 精品久久毛片 | 青娱乐导航 | 另类小说亚洲色图 | 91中文字幕在线 | 美女福利视频在线 | 国产干b| 亚洲欧洲自拍 | 亚洲欧洲日本在线 | 日韩人妻一区二区三区蜜桃视频 | 国产主播专区 | 葵司av在线| 又色又爽又黄无遮挡的免费视频 | 99久久久无码国产精品 | 欧美午夜在线 | 五月深爱 | 伊人情人综合 | 欧美亚洲另类在线 | 日韩在线视频免费播放 | 亚洲欧美色图片 | 日韩高清不卡一区 | 天天插天天插 | 成人黄色免费 | 日韩欧美国产激情 | 狠狠狠狠干 | 蜜桃av一区二区三区 | 麻豆videos| 国产欧美高清 | 天堂8在线 | 成人网站在线进入爽爽爽 | 极品丰满少妇 | 国产高清在线精品 | 久久久久久久久国产精品 | 桃色视频| 国产精品拍拍 | 图片区 小说区 区 亚洲五月 | 熟女一区二区三区四区 | 久久久久久999 | 色av网 | 亚洲国产欧美一区二区三区深喉 | 人人爽人人干 | 韩国三级中文字幕hd浴缸戏 | 新红楼梦2005锦江版高清在线观看 | xxxx69视频 | 久久牛牛 |